AL6XN vs 254 SMO
Aug 19, 2026
Ki diferans ki genyen ant AL-6XN ak 254 SMO?
AL-6XN vs . 254 SMO: Diferans prensipal la chita nan kontni nikèl; AL-6XN gen 23.5%-25.5% nikèl, tandiske 254 SMO gen 17.5%-18.5%. AL-6XN ofri rezistans siperyè nan krak korozyon estrès klori ak yon valè PREN yon ti kras pi wo (apeprè 46 kont 43) . 254 SMO prezante yon adisyon fè espre nan kòb kwiv mete (0.5%-1.0%) pou amelyore rezistans nan diminye korozyon asid epi li vini nan yon pri ki pi ba.
AL-6XN vs. 254 Gid Seleksyon SMO
| Egzijans | Materyèl Rekòmande | Rezon |
| Echanjeur chalè dlo lanmè (pi gran pase oswa egal a 40 degre) | AL-6XN | Pi wo PREN (~ 46 vs 43) ak pi wo Ni reziste klori SCC |
| Desulfurization gaz lafimen (FGD) | 254 SMO | Cu adisyon amelyore diminye rezistans asid; pri -efikas |
| Platfòm lanmè dife dlo / refwadisman | AL-6XN | Siperyè rezistans korozyon fant nan bride ak garnitur |
| Desalination RO manbràn lojman | AL-6XN | Pi wo evalyasyon presyon + SCC Marge nan Eau konsantre |
| klowòks kaka (anviwònman ClO₂) | 254 SMO | Dosye pwouve; pri avantaj sou AL-6XN |
| Bidjè-pwojè kontrent (mwens pase oswa egal a 35 degre dlo lanmè) | 254 SMO | Adekwat pèfòmans nan 10-15% pi ba pri |
| High-temperature service (>400 degre) | AL-6XN | ASME -apwouve a 427 degre vs ~ 400 degre pou 254 SMO |
| Pwojè mache Ewopeyen an (EN estanda) | 254 SMO | Gen deziyasyon EN 1.4547; AL-6XN se ASTM sèlman |
| Veso presyon (asme VIII koupon pou) | Swa | Tou de ASME-ki nan lis; AL-6XN gen pi wo estrès akseptab |
| Soudi diferan ak alyaj nikèl | AL-6XN | Pi wo baz Ni matche ak nikèl-filler alyaj pi byen |
Plant dessalement Mwayen Oryan: AL-6XN oswa 254 SMO?
Yon manadjè akizisyon nan yon plant dessalement Mwayen Oryan te mande yon fwa: "Tou de AL-6XN ak 254 SMO se 6-molybdène super austenitic Nerjaveèi. Fichye yo sanble prèske idantik. Poukisa yon sèl koute 10% plis, epi li aktyèlman gen pwoblèm pou pwojè mwen an?"
Sou papye, AL-6XN (UNS N08367) ak 254 SMO (UNS S31254) sanble ak marasa: tou de gen ~ 20% Kwòm, ~ 6% molybdène, ~ 0.2% Azòt, ak yon PREN pi wo a 40. Anpil founisè pral di ou yo "interchangeable." Yo pa.

Diferans kritik la chita nan kontni nikèl: AL-6XN pote 23.5–25.5% nikèl kont 254 SMO a 17.5–18.5%. Sis -pousantaj-pwen diferans sa a kondwi yon kaskad diferans pèfòmans - estrès korozyon rezistans krak, tolerans korozyon fant, limit tanperati, e menm disponiblite alontèm nan mache Ewopeyen an.
Chwazi sa ki mal, ak konsekans yo varye soti nan pitting akselere nan echanjeur chalè dlo lanmè a krak korozyon estrès klori nan echèk entèn scrubber FGD - ki koute 5-10 fwa diferans nan pri materyèl nan are san planifye.
Ki sa ki AL-6XN ak 254 SMO?
AL-6XN ak 254 SMO yo tou de 6-molybdène super austenitic Nerjaveèi - yon fanmi ki fèt pou konble diferans ki genyen ant estanda 316L ak alyaj nikèl chè tankou C-276. Yo reyalize valè PREN ki pi wo a 40 lè yo pouse molybdène ak nitwojèn nan limit la nan sa yon estrikti austenitic sèl-faz ka kenbe.
AL-6XN (UNS N08367)
- Non komès: AL-6XN® (mak anrejistre nan ATI Allegheny Ludlum)
- Nimewo UNS: N08367
- Estanda: ASTM A240, A312, A479, B688 (plak), B676 (soude tiyo),B675 (tiyo san pwoblèm), B564 (forge)
- Deziyasyon EN: Pa nan lis nan sistèm EN (ASTM-sèlman)
- Chimi kle: 20.5% Cr - 24% Ni - 6.3% Mo - 0.22% N
- Fòm komen: Plak, fèy, tiyo san pwoblèm, tiyo soude, ba, ekipman, bride, forgings.
- Devlopè: Allegheny Ludlum (kounye a ATI), te devlope nan kòmansman ane 1970 yo, te lanse komèsyalman an 1984.
- Pozisyon mache: Dominan nan Amerik di Nò; lajman espesifye nan veso presyon ASME-kode ak aplikasyon nikleyè

254 SMO (UNS S31254)
- Non komès: 254 SMO® (mak anrejistre nan Outokumpu Nerjaveèi)
- Nimewo UNS:S31254
- Estanda: ASTM A240, A312, A182 (klas F44), A269, A249, A813, A814; EN 1.4547
- EN deziyasyon: 1.4547 (X1CrNiMoCuN 20-18-6) - konplètman ki nan lis nan estanda Ewopeyen an
- Chimi kle: 20% Cr - 18% Ni - 6.1% Mo - 0.20% N - 0.7% Cu
- Fòm komen: Plak, fèy (bobin jiska 2m lajè), tiyo san pwoblèm, tiyo soude, ba, ekipman, bride, forgings.
- Devlopè: Avesta Jernverk (kounye a Outokumpu), Syèd, devlope nan ane 1970, komèsyal lanse 1982
- Pozisyon mache: Dominan nan Ewòp ak Azi; pi pito nan FGD ak desalination globalman
AL6XN VS 254 SMO: Konpozisyon chimik
| Eleman | AL-6XN (N08367) % | 254 SMO (S31254) % | Efè sou pèfòmans |
| Kabòn (C) | Mwens pase oswa egal a 0.030 | Mwens pase oswa egal a 0.020 | 254 SMO pi ba C diminye risk sansibilizasyon |
| Kwòm (Cr) | 20.0–22.0 | 19.5–20.5 | AL-6XN yon ti kras pi wo Cr → fim pasif ki pi estab |
| Nikèl (Ni) | 23.5–25.5 | 17.5–18.5 | KLE: AL-6XN a 6% pi wo Ni amelyore rezistans SCC |
| Molybdène (Mo) | 6.0–7.0 | 6.0–6.5 | AL-6XN pi wo ranje Mo → yon ti kras pi bon pitting |
| Azòt (N) | 0.18–0.25 | 0.18–0.22 | Tou de itilize N pou fòs + pitting |
| Kwiv (Cu) | Mwens pase oswa egal a 0.75 (rès) | 0.50–1.00 | 254 SMO Cu amelyore diminye rezistans asid |
| Manganèz (Mn) | Mwens pase oswa egal a 2.00 | Mwens pase oswa egal a 1.00 | AL-6XN pi wo Mn ede travayabilite cho |
| Silisyòm (Si) | Mwens pase oswa egal a 1.00 | Mwens pase oswa egal a 0.80 | Lower Si nan 254 SMO yon ti kras pi bon soudabilite |
| Fosfò (P) | Mwens pase oswa egal a 0.040 | Mwens pase oswa egal a 0.030 | 254 SMO pi sere P diminye soude cho fann |
| Souf (S) | Mwens pase oswa egal a 0.030 | Mwens pase oswa egal a 0.010 | 254 SMO ultra-low S amelyore soude/polisabilite |
| Fè (Fe) | Balans | Balans | Matris baz pou tou de |
Poukisa diferans Nikèl la pi enpòtan?
Diferans nikèl 6-pwen pousantaj (24% kont 18%) se sèl diferans ki pi enpòtan nan konpozisyon. Nikèl sèvi twa fonksyon kritik nan super austenitic asye pur:
- Estabilize austenite kont krak korozyon estrès klori (SCC). Papòt klasik pou iminite klori SCC nan asye pur austenitic se ~ 20% Ni nan tanperati ki pi wo a 60 degre. AL-6XN alèz depase sa a nan 24%; 254 SMO chita anba li nan 18%.
- Amelyore diminye rezistans asid.
- Ogmante duktilite metal soude.
AL6XN VS 254 SMO: Pwopriyete mekanik
| Pwopriyete | AL-6XN (N08367) | 254 SMO (S31254) | Jeni siyifikasyon |
| Fòs rupture (MPa) | Pi gran pase oswa egal a 690 (tip. 740–800) | Pi gran pase oswa egal a 650 (tip. 680–720) | AL-6XN ~ 10% pi wo → mens miray la |
| Sede fòs 0.2% (MPa) | Pi gran pase oswa egal a 310 (tip. 380–430) | Pi gran pase oswa egal a 300 (tip. 340–380) | Menm jan an; tou de ~ 2 × estanda 316L |
| elongasyon (%) | Pi gran pase oswa egal a 30 (tip. 45–50) | Pi gran pase oswa egal a 35 (tip. 40–50) | Tou de ekselan duktilite |
| Dite (HB) | Mwens pase oswa egal a 241 (tip. 200–220) | Mwens pase oswa egal a 223 (tip. 210) | Konparab; pi difisil pase 316L |
| Severite enpak (J, -196 degre) | Pi gran pase oswa egal a 70 | Pi gran pase oswa egal a 60 | Tou de ekselan nan tan kriyojenik |
| Modil Elastisite (GPa) | 200 | 195 | Prèske idantik |
| Dansite (g/cm³) | 8.04 | 8.00 | Diferans neglijab |
| Kondiktivite tèmik (W/m·K) | 11.9 | 14 | 254 SMO yon ti kras pi bon transfè chalè |
| Tanperati sèvis maksimòm (degre) | 427 (800 degre F, ASME) | ~400 (750 degre F) | AL-6XN pi wo ASME kòd temp |
| PREN (nominal) | ~46 | ~43 | AL-6XN pi wo rezistans pitting |
AL6XN VS 254 SMO: Rezistans korozyon
| Anviwònman | AL-6XN (N08367) | 254 SMO (S31254) | Gayan |
| Pitting klori (dlo lanmè anbyen) | CPT pi gran pase oswa egal a 85 degre (ASTM G48) | CPT Pi gran pase oswa egal a 80 degre | AL-6XN |
| Kowozyon nan fant (dlo lanmè, 40 degre) | CCT Pi gran pase oswa egal a 45 degre | CCT Pi gran pase oswa egal a 40 degre | AL-6XN |
| Dlo lanmè cho (pi gran pase oswa egal a 45 degre, kowonpi) | Ekselan | Bon (majinal) | AL-6XN |
| Klori SCC (80 degre, 1000 ppm Cl⁻) | Iminitè | Risk ki ba (Ni<20%) | AL-6XN |
| Sèvis sour H₂S (NACE MR0175) | Konfòme | Konfòme | Mare |
| Asid silfirik (dilye, mwens pase oswa egal a 20%) | Bon | Pi bon (Cu adisyon) | 254 SMO |
| Asid fosforik (pwosesis mouye) | Bon | Pi bon (Cu adisyon) | 254 SMO |
| Asid idroklorik (dilye, mwens pase oswa egal a 2%) | san Patipri | san Patipri | Mare |
| Asid nitrique (konsantre) | Bon | Bon | Mare |
| Caustik (NaOH, 50%) | Bon | san Patipri | AL-6XN |
| FGD kondansasyon (asid melanje + Cl⁻) | Bon (pitting) | Pi bon (inifòm) | Kontèks-depandan |
| High-temp oxidation (>500 degre) | Pa rekòmande | Pa rekòmande | Mare (itilize Ni alyaj) |
Sèvis Dlo Lanmè: Anviwònman k ap deside
Nan anbyen -tanperati dlo lanmè ap koule tankou dlo (mwens pase oswa egal a 35 degre), tou de alyaj fè ekivalan. Divèjans la kòmanse pi wo pase 40 degre oswa nan kondisyon kowonpi / fant:
- Pitting rezistans: Sèvi ak fòmil PREN (Cr + 3.3×Mo + 16×N), AL-6XN kalkile apeprè 46 kont 254 SMO a 43. Diferans 3 pwen sa a tradui nan yon avantaj tanperati kritik pitting (CPT) apeprè 5 degre pou AL-6XN. Nan pratik, AL-6XN reziste inisyasyon pitting jiska ~ 85 degre nan tès estanda ASTM G48, pandan y ap 254 SMO rive nan ~ 80 degre.
- Kowozyon nan fant: Pi gwo kontni nikèl AL-6XN nan ede kenbe estabilite fim pasif nan mikwo-anviwònman agresif nan fas bride, sifas garnitur, zòtèy soude, ak anba depo. Nan tès laboratwa pa ASTM G78, AL-6XN montre yon tanperati fant kritik (CCT) apeprè 5 degre pi wo pase 254 SMO.
- Estrès korozyon krak (SCC): Sa a se avantaj ki pi fò AL-6XN. ~24% kontni nikèl mete AL-6XN pi wo pase 20% Ni papòt jeneralman konsidere kòm nesesè pou iminite nan klori transgranulaire SCC nan asye pur austenitic . 254 18% Ni SMO a pi ba pase papòt sa a.

Sèvis Asid: Kote 254 SMO genyen
254 adisyon kwiv SMO a (0.5–1.0%) ba li yon avantaj mezirab nan diminye anviwònman asid. Nan sèvis FGD, fim nan kondansasyon sou sifas metal gen dilye H₂SO₄ melanje ak klori. Nan pwosesis mouye-asid fosfò, 254 SMO montre pi ba pousantaj korozyon inifòm pase AL-6XN, tipikman 0.1-0.3 mm/ane kont 0.2-0.5 mm/ane.
AL6XN VS 254 SMO: Pri
| Konpozan pri | AL-6XN (N08367) | 254 SMO (S31254) |
| Matyè premyè - plak (USD/kg) | 7.0–9.5 | 6.0–8.0 |
| Matyè premyè - tiyo san pwoblèm (USD/kg) | 12–22 | 10–18 |
| matyè premyè - ba (USD/kg) | 8–14 | 7–12 |
| Matyè premyè - ekipman (USD/kg) | 15–25 | 13–22 |
| Soudure consommables (USD/kg) | 45–65 (ERNiCrMo-3) | 45–65 (ERNiCrMo-3) |
| Pri fabrikasyon prim vs 316L | +30–50% | +25–40% |
| Lavi sèvis nan dlo lanmè (ane) | 20–30+ | 15–25 |
| Lavi sèvis nan FGD (ane) | 15–20 | 15–20 |
AL-6XN vs 254 SMO: Seleksyon Aplikasyon reyèl
Ka 1: Sistèm refwadisman dlo lanmè platfòm lanmè
Pwoblèm: Lanmè Nò platfòm lanmè, tanperati dlo lanmè 8-18 degre, men priz echanjeur chalè rive nan 45 degre. Sistèm gen 300+ koneksyon bride ki kreye sit fant. Kontni klori 19,000 ppm.
Rekòmande:AL-6XN
Rezon ki fè: Tanperati priz 45 degre konbine avèk sit fant nan flan yo kreye kondisyon egzak kote pi wo CCT AL-6XN ak pi wo nikèl (iminite SCC) bay yon maj sekirite desizif.
Ka 2: Desulfurization gaz lafimen (FGD) Scrubber
Pwoblèm: Chabon-izin elektrik FGD absòbe gwo kay won. Inlet gaz lafimen 150-180 degre, etenn a 60-80 degre. Kondansasyon gen dilye H₂SO₄ (5-15%), HCl (100-500 ppm), ak klori (10,000-30,000 ppm).
Rekòmande:254 SMO
Rezon ki fè: Konbinezon kondansasyon asid silfirik ak klori se 254 SMO a dous. Anplis de sa kòb kwiv mete bay rezistans siperyè nan eleman asid rediksyon an, pandan y ap 6% Mo okipe pitting klori. 254 SMO gen yon dosye pwouve 30+ ane nan plant Ewopeyen FGD.

Ka 3: Desalination RO Manbràn Lojman
Pwoblèm: Pliz-fach flash ak RO desalination plant nan Mwayen Oryan an. Eau segondè -presyon nan 40-60 degre, 70 bar presyon opere, klori konsantre (35,000-70,000 ppm).
Rekòmande:AL-6XN
Rezon ki fè: Konbinezon presyon ki wo, tanperati ki wo, ak sèl konsantre kreye yon menas trip: pitting, crevice, ak SCC. Pi gwo fòs sede AL-6XN ak iminite SCC nan ranje 40-60 degre se kritik.
Ka 4: Ekipman pou blanchi kaka ak papye
Pwoblèm: Kraft kaka moulen ClO₂ blanchi etap. Likid pwosesis la gen dyoksid klò, klori (500-2000 ppm), pH 2-4, tanperati 50-70 degre.
Rekòmande:254 SMO
Rezon ki fè: 254 SMO se estanda endistri a pou klowòks ClO₂. Nati oksidasyon ClO₂ pa benefisye de nikèl ki pi wo AL-6XN.
FAQ:
1. Ki diferans prensipal ant AL-6XN ak 254 SMO?
Diferans prensipal la se kontni nikèl: AL-6XN gen 23.5–25.5% Ni kont 254 SMO a 17.5–18.5% Ni. Sa a bay AL-6XN pi bon klori estrès korozyon krak rezistans ak yon ti kras pi wo PREN (~46 vs 43) . 254 SMO gen entansyonèl kwiv (0.5-1.0%) pou pi bon diminye rezistans asid epi li pote deziyasyon an EN 1.4547 pou pwojè Ewopeyen an.
2. Èske mwen ka itilize 254 SMO olye de AL-6XN nan dlo lanmè?
Wi, pou dlo lanmè anbyen-tanperati (mwens pase oswa egal a 35 degre) ki pa gen pwoblèm twou, tou de fè ekivalan. Pi wo pase 40 degre oswa nan sistèm ki gen anpil bride / garnitur, AL-6XN bay yon maj pi an sekirite.
3. Ki pi bon pou desulfurization gaz lafimen (FGD)?
254 SMO jeneralman pi pito pou scrubbers FGD paske adisyon kwiv li yo bay pi bon rezistans nan kondansasyon asid silfirik.
4. Èske AL-6XN ak 254 SMO se menm jan ak 904L?
Non. 904L (UNS N08904) se yon pi ba-molybdène (4–5% Mo) super austenitic ak PREN ≈ 36. AL-6XN ak 254 SMO tou de gen 6% Mo ak PREN > 42.
5. Ki metal filler mwen ta dwe itilize pou soude AL-6XN oswa 254 SMO?
Tou de alyaj sèvi ak ERNiCrMo-3 (Alloy 625 / Inconel 625) filler metal (AWS A5.14 ERNiCrMo-3 fil, AWS A5.11 ENiCrMo-3 elektwòd). Pou sèvis kritik, ERNiCrMo-4 (C-276 filler) bay pi wo maj korozyon. Pa janm sèvi ak filler ER316L oswa ER309L.
6. Èske AL-6XN oswa 254 SMO satisfè NACE MR0175 pou sèvis sour?
Wi, tou de alyaj yo ki nan lis nan NACE MR0175 / ISO 15156 pou sèvis tounen nan kondisyon rkwit ak dite mwens pase oswa egal a HRC 22. Ni pa egzije PWHT pou konfòmite sèvis tounen, depi kondisyon an kòm -livre se solisyon an rkwit.
7. Poukisa AL-6XN pi chè pase 254 SMO?
Pi gwo kontni nikèl AL-6XN (24% vs 18%) fè li pi sansib a pri nikèl LME. Nan pri nikèl aktyèl ($ 16,000-17,500 / tòn), siplemantè 6% Ni ajoute apeprè $ 1.00-1.50 / kg nan pri a matyè premyè.
8. Èske mwen ka soude AL-6XN nan 254 SMO?
Wi. Sèvi ak filler ERNiCrMo-3 (Inconel 625) pou jwenti ki diferan. Depo soude a pral gen chimi ant de metal debaz yo, ak bon jan rezistans korozyon. Pa gen okenn prechofe espesyal oswa PWHT obligatwa.
9. Ki limit tanperati AL-6XN vs 254 SMO?
AL-6XN ASME apwouve jiska 427 degre (800 degre F); 254 SMO anjeneral limite a ~ 400 degre (750 degre F). Tou de pa ta dwe itilize pi wo a 500 degre akòz risk sigma faz frajilman.
10. Èske 254 SMO gen yon deziyasyon estanda EN?
Wi, 254 SMO nan lis EN 1.4547 (X1CrNiMoCuN 20-18-6) nan sistèm estanda Ewopeyen an. Sa fè li konplètman konfòme ak PED 2014/68/EU pou ekipman presyon nan mache Ewopeyen an. AL-6XN pa gen yon deziyasyon EN - li se yon klas ASTM sèlman.